date: 2025-04-11 17:34
---
#semiconductor #dssc
教科書では
- tio2 3g
- 純水 7g
- PEG 1g
今村さんいわく、最初はサラサラだが30分混ぜ続けるとペースト状になってくる
## 材料
- 酸化チタンパウダー [Amazon | 吉祥 日本画用絵具 粉末絵具 チタン白 500g | 絵具 通販](https://www.amazon.co.jp/%E5%90%89%E7%A5%A5-%E6%97%A5%E6%9C%AC%E7%94%BB%E7%94%A8%E7%B5%B5%E5%85%B7-%E7%B2%89%E6%9C%AB%E7%B5%B5%E5%85%B7-%E3%83%81%E3%82%BF%E3%83%B3%E7%99%BD-500g/dp/B001MS8420?th=1) 5g
- 純水(モノタロウ) 10.1g
- AcAc(氷酢酸) 0.2g
- PEG200 [ポリエチレングリコール 200(研究実験用) 1本(500g) 林純薬工業 【通販モノタロウ】](https://www.monotaro.com/p/3141/9833/) 1.5g
合計5/16.6  なので30.1204819 Wt% 濃度は合ってる
が、1時間半やっても全然クリーム状にならず。その後放置したのを見てみたら普通に沈殿していた
結局、
- tio2 3g
- AcAc 0.5g
- PEG 1g
でまずネチネチの状態でしばらく練り、水 0.35gを加えて緩めた。
これぐらいでちょうどよかった(これでも比較的緩い)
ちゃんとナノサイズのパウダーを使うと水と混ぜるだけでも十分いいペースト状になるらしいとのことで、画材のチタン白の粒度が荒いのだろうか?
最終的な[[簡易的な粘度測定|粘度を定量化]]するのがよいのかもしれない。
とりあえずこれをガラスアプリケーターで塗る。メンディングテープ